Articles

How lithium-ion charging works: CC/CV, the charge curve and the terms

A lithium-ion cell charges in two main phases, constant current then constant voltage (CC/CV). First the charger holds a constant current, typically 0.5C for an energy cell and 1C or more for a power cell, while the cell voltage climbs. When the voltage reaches the cell’s charge voltage, 4.2 V for most cells, 4.35 or 4.4 V for high-voltage cells and 3.6 to 3.65 V for LiFePO4, the charger holds that voltage and the current tapers away. Charging stops when the current falls to a termination level, which cell datasheets put at 0.02C to 0.05C. A deeply discharged cell gets a small precharge current first, and charging is only allowed inside a temperature window, often 0 to 45 °C. Unlike NiMH or lead-acid, a full lithium-ion cell normally gets no float or trickle charge afterwards.

Every charger for a lithium cell, from a single-chip charger on a wearable to a firmware-run charger on a large pack, is built around those phases. Electrically it’s a current-limited voltage source, with precharge, termination, timers and temperature checks around it. This article defines the terms and walks through the charge curve one phase at a time; a companion article works each setting at its worst-case tolerance, which is where chargers that pass on the bench go wrong in the field.

I’ve designed chargers from small single cells up to custom multi-cell packs of around 30 V, lithium-ion and LiFePO4, including chargers built from discrete parts with the charge control and protection in my own firmware. The same few phases sit underneath all of them.

The terms

Battery datasheets and charger datasheets use a small vocabulary, and a few of the words mean less than they seem to.

Term What it means What to watch
Capacity (mAh, Ah) The charge a cell delivers from full down to its cutoff voltage, at the discharge current and temperature the datasheet states Rated under kind conditions. At a heavy load or in the cold, you get less.
Energy (Wh) Charge times voltage over the discharge; roughly capacity times nominal voltage Comparing mAh only works between cells or packs of the same nominal voltage.
Nominal voltage The average voltage over a discharge: about 3.6 V for most lithium-ion, higher for high-voltage cells, and 3.2 to 3.3 V for LiFePO4 It’s for working out energy. It isn’t a limit.
Charge voltage The voltage the charger holds in the constant-voltage phase: the most the cell is charged to Its accuracy matters as much as its value.
Cutoff voltage The voltage where the rated discharge ends, often 2.5 V on lithium-ion datasheets Most products shut down well above it.
C-rate Current relative to capacity: 1C for a 2 Ah cell is 2 A, 0.5C is 1 A A rate quoted without the capacity it refers to means nothing.
State of charge The charge left, as a share of full Hard to measure; voltage is only a rough guide.
Depth of discharge The share of capacity used in a cycle It affects cycle life, by an amount that depends on the cell.
Internal resistance The voltage drop per amp of current through the cell It changes with state of charge, temperature and age. Datasheets often quote a 1 kHz AC figure, which is lower than the DC resistance that sets heating and voltage sag.
Open-circuit voltage The cell’s voltage at rest, with no current The voltage at the terminals differs from it whenever current flows.
Cycle life Full cycles until capacity falls to a stated share of rated, under stated conditions The conditions (rate, depth, temperature, charge voltage) are the whole story.
Calendar life Aging with time, whether the cell is used or not Worse when stored full or hot.
Coulombic efficiency Charge out divided by charge in Above 99 percent on a healthy cell.
Energy efficiency Energy out divided by energy in Lower than coulombic efficiency, because the cell charges at a higher voltage than it discharges at.
Self-discharge Charge lost while the cell sits unused Small, but it adds up over months, and faster when warm. Protection circuits and dividers on the cell add to it.
Precharge (trickle) A low current used before fast charging to bring up a deeply discharged cell Lithium charger datasheets often call it trickle charging.

Two of these trip people up more than the rest. Capacity is defined on discharge, under specific conditions, so the charge you count going in during charging isn’t the rated capacity, even though the two are close. And terminal voltage isn’t the cell’s voltage: while current flows in, the terminals sit above the open-circuit voltage by the current times the internal resistance, and while it flows out, below it. That one relationship explains a lot of the charge curve.

“Trickle” causes its own confusion. On NiMH and lead-acid it means a small continuous current that keeps a full battery topped up. On lithium-ion charger datasheets the same word usually means the precharge phase at the start of a charge. A lithium cell gets that low current when it’s nearly empty and never as a continuous charge once it’s full.

All of these numbers are per cell. A pack of cells in series multiplies the voltages by the number of cells and keeps the capacity in amp-hours of one cell; cells in parallel add capacity and keep the voltage.

Worked through for one example cell: a 3 Ah lithium-ion cell with a nominal 3.6 V holds about 10.8 Wh. A 0.5C charge is 1.5 A. A termination at 0.02C is 60 mA, and at 0.05C it’s 150 mA. Three of them in series make a 10.8 V, 3 Ah pack of 32.4 Wh, charged to 12.6 V.

For the discharge side, usable capacity at real loads and temperatures and how to measure it, see Battery-powered design: budgeting and measuring power. The battery life calculator turns a cell’s capacity and a product’s modes into an estimate.

The charge curve

Lithium-ion charge curve: precharge, constant current, constant voltage, terminationTime runs left to right. During a short precharge the current is small and the voltage rises from deeply discharged to the precharge threshold. Then the current steps up to a constant level while the voltage climbs, quickly at first, then fairly steadily, until it reaches 4.2 volts. From there the voltage is held at 4.2 volts and the current tapers down until it reaches the termination level, when charging stops and the voltage relaxes slightly. The area under the current curve is shaded and labelled as the charge put in, the integral of current over time.PreConstant currentConstant voltageDoneCharge put inarea under the current, Q = ∫ I dtCell voltageCurrentTime4.2 V charge voltagePrecharge thresholdTermination currentCurrent tapersVoltagerelaxes
One example cell charging from deeply discharged to full. The current (orange) is held constant until the voltage (white) reaches the charge voltage, then tapers while the voltage is held, and the charge stops at the termination current. The shaded area under the current curve is the charge put in. Illustrative shape, not to scale.

The figure follows one cell from deeply discharged to full. The proportions are illustrative. Read it as two traces against time: the voltage at the cell’s terminals, and the current flowing into it.

The area under the current curve

The charge put into a cell is the current integrated over time, Q = ∫ I dt. On the figure that’s the shaded area under the current trace. A steady 1 A for one hour is 1 Ah. A current that tapers in a straight line from 1 A to zero over an hour is half that, 0.5 Ah, because the area under it is a triangle. Real tapers aren’t straight lines, but the idea is the same: what the cell has received is the area, not the current at any moment.

Energy is the same integral with voltage in it: E = ∫ V · I dt, in watt-hours. Because the voltage is higher late in the charge than early on, an amp-hour added near the end carries more watt-hours than one added at the start.

Almost all of the charge comes back out on a healthy cell; the coulombic efficiency of a well-made cell measured at a low rate is 99.8 percent or more, and above 99 percent is a safe working figure. What’s lost is energy, not charge. The cell charges at a voltage above its resting voltage and discharges below it, the difference being the current times the internal resistance plus a small hysteresis in the chemistry, so some of the energy put in turns to heat. That’s why a cell warms a little on charge, more at higher current, and why energy efficiency is lower than coulombic efficiency.

Precharge

A cell below a precharge threshold, typically 2.5 to 3.0 V on lithium-ion chargers (about 2 V on LiFePO4 chargers), gets a reduced current, often 10 to 20 percent of the fast-charge current, until its voltage passes the threshold. Both numbers are charger settings with their own tolerances, and the spread across chargers is wider than the typical values; the article on control points and tolerances works through them. A cell that low has usually been run down hard or left discharged, and a gentle current brings it up without stressing it while the charger watches whether it responds. If the voltage doesn’t rise within a set time, typically somewhere between half an hour and a few hours, a precharge timer stops the charge, because a cell that won’t come up is a cell to distrust. Many chargers also have a lower, battery-short threshold, around 1.6 to 2.35 V for lithium-ion and nearer 1.2 V for LiFePO4, below which they feed a fixed small current or nothing. That current ranges from a few milliamps on small linear chargers to around 100 mA on some switching chargers, which is a lot for a small damaged cell. In a pack, the protection circuit may also have disconnected an over-discharged cell, so the charger sees nothing until it applies a voltage that lets the protection reconnect.

Precharge is meant for a cell that has run down to around its rated cutoff. A cell that has gone well below its end-of-discharge voltage is a different case. The JEITA guideline on lithium-ion batteries in notebook computers and tablets advises against charging it, because the negative electrode’s copper current collector can dissolve when a cell is driven down toward 0 V, and on recharge that copper can deposit where it can grow into an internal short. Cell makers also advise recharging a stored cell before it drifts down to its cutoff. Where the floor sits, and whether the charger or the protection circuit enforces it, is a design decision with a safety side to it.

Constant current

Above the precharge threshold the charger delivers its full charge current and holds it. Cell datasheets give a standard charge current, often 0.5C and sometimes as low as 0.2C, and a maximum, often 1C. Power cells are rated higher, around 2C for some, and some LiFePO4 power cells allow 4C to 80 percent charge. The voltage rises through this phase: quickly at first, out of the low end, then fairly steadily up to the charge voltage. (A LiFePO4 cell is different: flat for most of the charge, then a steep rise at the end.)

The terminal voltage during this phase is the open-circuit voltage plus the current times the internal resistance. So a higher charge current, or a cell with more resistance (an aged or cold one), reaches the charge voltage sooner, at a lower state of charge, and leaves more of the charge for the slower constant-voltage phase. That’s why doubling the charge current doesn’t halve the charge time. The same applies to any resistance between the charger and the cell: the charger regulates the voltage at its own output, so a protection switch, a connector or a long lead adds its drop to the cell’s and moves the switch to constant voltage earlier.

On a linear charger, the heat in the charger is the input voltage minus the cell voltage, times the current, so it’s highest at the start of the constant-current phase, when the cell voltage is lowest. That’s where a charger’s thermal regulation most often trims the current.

Constant voltage

When the terminal voltage reaches the charge voltage, the charger switches to holding that voltage. The cell’s open-circuit voltage keeps rising toward it, so the difference across the internal resistance shrinks and the current falls away on its own. The constant-voltage phase delivers the last part of the charge, and it can take as long as the constant-current phase while adding much less of it.

The charge voltage has to be accurate. A cell datasheet might give 4.20 V ± 0.05 V, and charger datasheets specify how closely they hold their setting, typically within 0.5 to 1 percent, which is 21 to 42 mV at 4.2 V. What has to stay under the cell’s limit is the charger’s maximum, not its setting. On a high-voltage cell whose 4.35 V is an absolute maximum, a charger set to 4.35 V with ±0.75 percent tolerance can go 33 mV over it, so the setting has to sit below the limit by at least the tolerance.

Charging above the limit speeds up aging and, further above it, risks lithium plating and electrolyte breakdown, which is a safety problem as well as a lifetime one. Charging below it gives up capacity and usually, though not always, gains life. How much of each depends on the chemistry and the cell, so the cell maker’s figures at the chosen voltage are the ones to use; the rules of thumb that circulate online don’t hold across cells.

Termination, and why there’s no float

The charge ends when the current tapers to the termination level. Cell datasheets state their own cutoff, typically 0.02C to 0.05C, and charger chips often default to a tenth of the programmed charge current, with options down to a few percent. A tenth of the charge current isn’t 0.1C: at a 0.5C charge it’s 0.05C, inside the cell makers’ range, but at 1C it’s 0.1C, which stops the charge earlier than the datasheet’s capacity figure assumes. A lower termination current adds a little capacity and a lot of time, and a charger’s termination accuracy is at its worst at low settings.

After termination the charger stops. It doesn’t hold the cell at full voltage or keep feeding it a trickle, which is the opposite of how NiMH and lead-acid are treated. A lithium-ion cell has no safe way to absorb overcharge, and time spent at full voltage ages it faster, so continuous current into a full cell does harm with nothing to show for it. Instead the charger watches the voltage, and if it falls by more than a recharge threshold, typically 100 to 200 mV below the charge voltage (roughly 60 to 265 mV across chargers and settings, more on some that set it as a percentage), it charges again. A product that runs from its charger while the cell sits full needs a charger with a power path, which feeds the system from the input and leaves the cell disconnected after termination. Without one, the load sits on the cell, the charger may never see the current fall to its termination level, and the cell is effectively held at full voltage. Even with a power path, a cell kept full and warm in a powered product ages faster than one kept part-charged. LiFePO4 is a partial exception: one LiFePO4 cell maker gives a float voltage, a little below the charge voltage, for standby use.

Most chargers also run a fast-charge safety timer, typically 5 to 20 hours, alongside the shorter precharge timer, so a cell that never reaches termination, because of a fault or a load drawing current through the charger, isn’t charged forever. Some simple chargers have no timer at all. Many chargers suspend termination while they’re limiting the current because the charger chip itself is hot or the input is weak, or while the cell is in a cool or warm temperature band, and some slow their timer at the same time, which is one way a charge runs far longer than expected.

After charging stops

The voltage drops a little once the current stops, as the figure shows. Part of the drop is the current times the internal resistance, and that part goes the instant the current stops; at a termination current of a few hundredths of C it’s small. The rest is polarization inside the electrodes and electrolyte, which relaxes over minutes to hours as the lithium concentration evens out. The drop is larger if the charge is cut off early at high current, by a timer or by unplugging. It’s normal, and it isn’t the cell losing charge, but it has to stay inside the recharge threshold, or the charger starts a new charge soon after finishing one. It’s also why a voltage read straight after charging, or under load, overstates or understates the state of charge.

Temperature

Lithium-ion cells may only be charged inside a narrower temperature range than they discharge over. Many cell datasheets give 0 to 45 °C for charging against -20 to 60 °C for discharging, measured at the cell’s surface, not the board’s; some power cells allow charging to 60 °C, and some cells ask for a reduced current below 10 °C. Chargers with a cell temperature input often follow the zones in the JEITA guideline: a standard range where the full current and voltage apply, a cool band with reduced current, a warm band with reduced voltage (and often current), and no charging outside them. The guideline defines the zones; the temperatures and reductions are set per cell, and the 0, 10, 45 and 60 °C edges found on many chargers are implementations, not the guideline’s values. Basic chargers may have only a hot and cold cutoff, or no cell temperature input at all. Charging a standard lithium-ion cell below freezing can plate metallic lithium on the negative electrode, which permanently reduces capacity and can grow into an internal short. Some cells are rated for slow charging below 0 °C, among them some LiFePO4 cells, at a reduced current, and some lithium titanate cells, which their makers rate for charging at a reduced current well below freezing, so the datasheet decides. The temperature article covers thermistor placement and what to do in the cold.

Chemistries

“Lithium-ion” is a family. The cathode chemistry sets the voltages, and one anode type changes them again.

Type Charge voltage per cell Nominal per cell What sets it apart
Cobalt-oxide, nickel-manganese-cobalt, nickel-cobalt-aluminium, manganese-oxide 4.2 V about 3.6 V The long-established types, in tools and many products
High-voltage variants 4.35 or 4.4 V higher Higher energy density; some datasheets state the charge voltage as an absolute maximum
Iron phosphate (LiFePO4) 3.6 to 3.65 V 3.2 to 3.3 V Long cycle life, flat voltage curve, lower energy density
Lithium titanate (anode) about 2.8 V about 2.4 V Very high charge rates, wide temperature range, very long cycle life, low energy density
Discharge curves: standard lithium-ion against LiFePO4Cell voltage against the charge delivered, from full on the left to empty on the right. The standard lithium-ion curve starts high and slopes down steadily across the whole discharge before dropping at the end. The LiFePO4 curve starts lower, drops briefly, then stays almost flat across most of the discharge, and falls steeply only at the very end.Cell voltageFullEmptyCharge deliveredStandard lithium-ion: falls steadilyLiFePO4: almost flat for most of its capacity
Discharge curves of two lithium-ion chemistries. A standard 4.2 V lithium-ion cell's voltage falls steadily, so voltage says roughly how much charge is left. A LiFePO4 cell holds an almost flat voltage across most of its capacity, so voltage says very little until it is nearly full or nearly empty. Illustrative shapes, not to scale.

The shape of the discharge curve matters to the charger as well as to the product. A standard 4.2 V lithium-ion cell’s voltage falls steadily as it discharges, so voltage is a rough guide to the charge left. LiFePO4 sits on an almost flat plateau across most of its capacity, so voltage tells you very little until the cell is nearly full or nearly empty. That affects how a LiFePO4 charger sees the end of charge and how a pack of them is balanced.

For contrast, the two older rechargeable chemistries are charged differently:

  • NiMH is charged at constant current, and the end of charge is detected by a small drop in voltage, a few millivolts per cell, or by the temperature rising at a degree or two per minute as the cell fills, backed by a timer. A maintenance trickle afterwards is common, at a rate the cell maker sets, anywhere from about C/300 to C/20; one maker allows it only after a full charge and with a timer.
  • Lead-acid is charged at constant current, then held at about 2.40 to 2.50 V per cell for cyclic use, or kept at a float voltage of 2.25 to 2.30 V per cell for standby, where it can stay for long periods. Both figures are for 25 °C and come down as the battery warms, so lead-acid chargers compensate for temperature.

Primary lithium cells, such as lithium coin cells, aren’t rechargeable, and charging one, even through a leakage path nobody intended, can make it vent or catch fire.

How long a charge takes

At the standard 0.5C rate, cell datasheets quote three to four hours for a full charge. A power cell rated for faster charging may quote an hour and a half, and a LiFePO4 power cell charged at 1C quotes 45 minutes. Charging slows near full because the constant-voltage phase takes the last part of the charge at a falling current: on one datasheet’s four-hour standard charge, the constant-current phase at 0.5C can’t account for more than about two hours, so the taper takes the rest. A higher current shortens the first phase and not the second, and a charger limited by a weak source or its own temperature stretches both.

If you’re choosing a charger for a lithium product, or designing one, and want the numbers checked against the cell’s datasheet, get in touch.

All articles

Have a project in mind?

Based in southern Indiana. Working with clients anywhere, including companies across the Midwest.